Revealer 3D-DIC Measurement of the Nonlinear Viscoelastic Poisson’s Ratio of NEPE Solid Propellant: A Multiscale Mechanistic Study

Table of Content [Hide]

    Abstract

    In this study, a Revealer 3D-DIC system was employed to measure the macroscopic strain and Poisson’s ratio of NEPE solid propellant during tensile loading, stress relaxation, and cyclic loading. It was found that the Poisson’s ratio decreases from an initial value of approximately 0.495 with increasing strain, falling to 0.35 at approximately 60% strain. Combined with SEM, CT, and RVE analyses, the study links this macroscopic evolution to the propagation of particle–matrix interfacial debonding, and demonstrates the necessity of accounting for the nonlinearity of Poisson’s ratio in multiscale constitutive models.

     

    Experimental Background

    NEPE (nitrate ester plasticized polyether) solid propellant is a class of highly filled polymer-matrix composite material exhibiting viscoelasticity and large-deformation behavior. Under load, interfacial debonding, crack propagation, and void evolution may occur between the binder matrix and the solid particles, thereby altering the macroscopic mechanical response of the material. Poisson’s ratio characterizes the relationship between longitudinal and transverse deformation; its evolution affects calculations of the volumetric response and damage evolution.


    This study focuses on the nonlinearity and time dependence of the Poisson’s ratio of NEPE propellant, examining its variation under different temperatures, strain rates, and loading paths (tension, relaxation, and cyclic loading), and exploring the connection between the macroscopic evolution of Poisson’s ratio and microstructural damage. By combining macroscopic deformation measurements from stereo (dual-camera) 3D-DIC with scanning electron microscopy (SEM), X-ray computed tomography (CT), and representative volume element (RVE) simulations, the study provides experimental and modeling references for the mechanical analysis of solid propellants and other particle-filled composites.

     

    Experimental Setup: Stereo 3D-DIC and Microstructural Characterization

    The macroscopic mechanical tests were conducted on a universal testing machine equipped with an environmental chamber. Black speckle patterns were applied to the surfaces of the NEPE specimens for digital image correlation. The load and displacement were acquired by the machine’s internal sensors at 50 Hz, and the specimens were imaged in stereo by the Revealer 3D-DIC system through the optical glass window of the environmental chamber.


    The Revealer 3D digital image correlation system consists of two synchronized cameras equipped with 50 mm focal length lenses; each camera has a resolution of 4096 × 3000 pixels and a maximum acquisition rate of 20 fps. The displacement measurement accuracy reported in the original study is better than 0.01 pixels, and the strain measurement accuracy is better than 20 με. The system was used to track longitudinal and transverse gauge-length markers for Poisson’s ratio calculation; in the center-hole specimen tests, it was used to obtain full-field surface strain distributions.

     

    revealer-3d-dic-measurement-of-the-nonlinear-viscoelastic1.jpg 

    Figure1. Tensile test configuration inside the environmental chamber and the layout of the dumbbell-shaped specimen. The specimen is clamped in the testing machine, and two Revealer 3D-DIC cameras synchronously acquire images of the specimen surface from different viewing angles; the schematic on the right shows the specimen gauge section, geometric dimensions, and coordinate axes.

     

    Microstructural characterization was performed by SEM observations of the specimen surfaces at different deformation stages, and the internal voids were reconstructed by industrial CT. The microstructural information provided by SEM and CT is complementary to the macroscopic deformation data measured by DIC.

     

    Test Methods: Tensile Loading, Stress Relaxation and Cyclic Loading

    The specimens included standard dumbbell-shaped tensile specimens, rectangular specimens for microscopic observation, and center-hole specimens for validation. The dumbbell specimens had a gauge length of 70 mm and a cross-section of 10 mm × 10 mm; the center-hole specimens measured 100 mm × 30 mm × 10 mm with a 10 mm diameter central through-hole. The NEPE formulation studied contains ammonium perchlorate (AP, approximately 15 wt%), HMX (octogen, approximately 40 wt%), aluminum powder (approximately 20 wt%), and other constituents.


    The uniaxial tensile tests covered temperatures of 10, 25, 40, and 60 °C, and strain rates of 2.38 × 10⁻⁴, 2.38 × 10⁻³, and 1.19 × 10⁻² s⁻¹. The stress relaxation tests were performed at 25 °C: the specimens were stretched stepwise to 14 mm, with each step followed by a 1800 s hold after every 7 mm displacement increment. The cyclic loading tests adopted a loading–unloading path with progressively increasing displacement amplitudes, with three cycles per level. Each test condition was repeated at least five times, and the dataset closest to the mean was selected for subsequent analysis.


    Poisson’s ratio was calculated using the DIC extensometer method, in which the system tracks the displacement of longitudinal and transverse gauge-length markers to obtain the corresponding strains.


    The DIC image analysis used a subset of 49 pixels, a step size of 7 pixels, and a 7 × 7 Gaussian filter, with a calibration scale of 0.040 mm/pixel. Image acquisition was configured according to the test stage in the original study: approximately 1500, 4000, and 10,000 images were acquired for the uniaxial tension, relaxation, and cyclic tests, respectively. Near fracture, localized large deformation may degrade the speckle correlation quality; consequently, the maximum strain obtained by DIC may be lower than that derived from the testing machine displacement conversion.


    The center-hole specimens were tested at 25 °C and 10 mm/min. The test paths included stretching to 25 mm, and stretching to 15 mm followed by a 1800 s hold. The longitudinal strain full-fields obtained by 3D-DIC were used for comparison with the strain fields from finite element simulation.

     

    Experimental Data Analysis: Macroscopic Deformation and Poisson’s Ratio Measured by 3D-DIC

    Decrease of Poisson’s Ratio with Strain During Tension

    The stress–strain curves in the uniaxial tensile tests were obtained from the testing machine load and displacement data, while the Poisson’s ratio–strain curves were computed from the longitudinal and transverse gauge strains tracked by 3D-DIC. In the initial small-strain stage, the longitudinal strain is small and the Poisson’s ratio fluctuates slightly; with increasing strain, the Poisson’s ratio decreases approximately linearly. The initial Poisson’s ratio is approximately 0.495, approximately 0.37 at 50% strain, and decreases to 0.35 at approximately 60% strain. The Poisson’s ratio curves under different temperatures and strain rates are generally similar, indicating that, within the tested range of this study, temperature and strain rate have no pronounced effect on the Poisson’s ratio of the NEPE propellant, and the deformation level is the dominant factor.


    revealer-3d-dic-measurement-of-the-nonlinear-viscoelastic2.jpg 

    Figure2. Uniaxial tensile results of the NEPE solid propellant. (a) Stress–strain curves obtained from the testing machine data at different temperatures and strain rates; (b) Poisson’s ratio–strain curves computed from the 3D-DIC longitudinal and transverse strains. The Poisson’s ratio decreases from an initial value of approximately 0.495 with increasing strain, reaching approximately 0.35 at about 60% strain; the curves are generally consistent across the test conditions.

     

    Slight Recovery of Poisson’s Ratio During Stress Relaxation

    In the stepwise stretch-and-hold stress relaxation tests, the stress decays with time, while the Poisson’s ratio computed from 3D-DIC increases slightly during the hold periods, with a more pronounced change at the onset of relaxation that gradually stabilizes thereafter. During the first relaxation period, the longitudinal strain decreases by approximately 0.3%, and the transverse strain increases by approximately 0.12%. The out-of-phase evolution of the two strain components during the hold reflects the viscoelastic strain hysteresis of the material, and corresponds to the transient recovery of Poisson’s ratio during the relaxation stage.


    revealer-3d-dic-measurement-of-the-nonlinear-viscoelastic3.jpg 

    Figure3. Stress and Poisson’s ratio versus time during stress relaxation. The blue curve denotes the stress measured by the testing machine, and the red curve denotes the Poisson’s ratio computed from the 3D-DIC strains; after entering the displacement hold stage, the stress decays, while the Poisson’s ratio recovers slightly and gradually stabilizes.

     

    revealer-3d-dic-measurement-of-the-nonlinear-viscoelastic4.jpg 

    Figure4. Longitudinal and transverse strain–time curves measured by 3D-DIC during the first stress relaxation period. During the hold, the longitudinal strain gradually decreases while the transverse strain evolves toward zero; the out-of-phase evolution of the two strain components reflects the viscoelastic strain hysteresis of the NEPE propellant.

     

    Ratcheting Evolution of Poisson’s Ratio Under Cyclic Loading

    During cyclic loading, the Poisson’s ratio decreases overall with accumulated total strain, and the residual strain after unloading accumulates progressively. Taking the three cycles at the 42 mm displacement level as an example, the evolution trends of Poisson’s ratio during loading and unloading are essentially consistent; as cycling proceeds, both the upper envelope of the Poisson’s ratio and its post-unloading value decrease progressively, exhibiting a ratcheting-type evolution. The cyclic stress response exhibits softening, whereas the loading and unloading branches of the Poisson’s ratio evolve in a similar manner, showing no pronounced Mullins effect. Therefore, the Mullins effect and the ratcheting effect should be assessed separately with respect to the specific response variables.

     

    revealer-3d-dic-measurement-of-the-nonlinear-viscoelastic5.jpg 

    Figure5. Poisson’s ratio–strain curves of the NEPE solid propellant during cyclic loading–unloading. (a) Evolution of Poisson’s ratio over the complete cyclic test; (b) local curves of the three cycles at the 42 mm displacement level. The Poisson’s ratio decreases progressively with strain and cycle number, and the loading and unloading branches exhibit similar trends.

     

    revealer-3d-dic-measurement-of-the-nonlinear-viscoelastic6.jpg 

    Figure6. Residual strain and Poisson’s ratio after unloading versus cycle number. The residual strain accumulates progressively, reaching approximately 7.5% at the end of the test, while the post-unloading Poisson’s ratio decreases approximately linearly with the number of cycles.

     

     

    Full-Field Strain Prediction Validated on Center-Hole Specimens

    A central hole induces localized strain concentration. The Revealer 3D-DIC system measured the full-field longitudinal strain on the surface of the center-hole specimens, which was compared against finite element simulation results. Under tension, the circular hole deforms into an ellipse; a pronounced strain response appears near the minor-axis direction of the hole, whereas the strain response near the major-axis direction is weaker. At a specimen displacement of 15 mm, the maximum longitudinal strain is approximately 39%; at 25 mm, it is approximately 59%. The original study notes that the high-strain regions correspond to the locations where specimen failure initiates. The distribution of the DIC-measured strain field agrees well with the simulation, providing experimental validation of the constitutive model’s deformation prediction under complex stress states.


    revealer-3d-dic-measurement-of-the-nonlinear-viscoelastic7.jpg 

    Figure7. Comparison between the DIC strain fields and the finite element simulation results for the center-hole specimen under tension. (a) Longitudinal strain contour at a displacement of 15 mm, with a maximum strain of approximately 0.39; (b) longitudinal strain contour at 25 mm, with a maximum strain of approximately 0.59; in each panel, the left side shows the DIC experimental result and the right side the simulation result; © stress distribution from the finite element computation at 25 mm. Both the DIC and simulation results reveal strain concentration around the hole.

     

    Macroscopic DIC Results and Microscopic Damage Mechanisms

    The 3D-DIC measurements provide the surface strain field of the specimen and the Poisson’s ratio computed from the longitudinal and transverse strains. The particle–matrix interfacial separation displacement, internal crack length, and void volume fraction were analyzed by SEM, CT, and RVE simulations, and should not be regarded as direct DIC measurement results.


    The RVE simulations show that the decrease in Poisson’s ratio occurs mainly in the cohesive-zone propagation stage after the particle–matrix interface enters the damaged state, and decreases with increasing interfacial separation displacement. Based on this, the study selected variables such as the normalized interfacial separation, crack length, and volume ratio to construct a multiscale constitutive model, implemented via an ABAQUS UMAT subroutine. The full-field strain results from DIC on the center-hole specimens provided experimental validation for this model. Accordingly, the 3D-DIC measurements, microscopic characterization, and RVE simulations respectively fulfill the roles of macroscopic deformation quantification, microstructural observation, and mechanistic interpretation.

     

    Key Findings: Nonlinear Poisson’s Ratio and the Role of 3D-DIC Measurement

    • Under the NEPE propellant formulation and test conditions of this study, the Poisson’s ratio measured by the Revealer 3D-DIC system decreases approximately linearly with tensile strain, from an initial value of approximately 0.495 to 0.35 at approximately 60% strain; variations in temperature and strain rate did not produce significant differences in Poisson’s ratio.

    • During stress relaxation, both the longitudinal and transverse strains evolve with time with a hysteresis, and the Poisson’s ratio recovers slightly before stabilizing. Under cyclic loading, the Poisson’s ratio exhibits ratcheting-type decay; the original study observed cyclic softening in the stress response, but no pronounced Mullins effect in the Poisson’s ratio.

    • The 3D-DIC full-field strain results on the center-hole specimens reveal strain concentration around the hole and agree well with the finite element strain fields, validating the model’s capability to predict the deformation response under complex loading.

    • The link between particle–matrix interfacial propagation and the decrease in Poisson’s ratio derives from SEM, CT, and RVE analyses. The multiscale constitutive computations show that neglecting the nonlinearity of Poisson’s ratio underestimates the bulk modulus degradation and overestimates the shear modulus degradation, and underestimates the volume after deformation.


    This study provides an experimental case for measuring the macroscopic strain and Poisson’s ratio of solid propellants under large deformation, stress relaxation, and cyclic loading by 3D-DIC, and offers a reference for the multiscale analysis of particle-filled polymer-matrix composites.

    References
    Quick Links
    Contact Us
    Email:
    sales@revealerhighspeed.com
    Add:
    Fuhuang Intelligent New Vision Building, Baohe District, Hefei City, China.
    Quick Links
    Add:
    Fuhuang Intelligent New Vision Building, Baohe District, Hefei City, China.